Analysis of Short Circuit Fault Caused by soft pack Lithium Battery, how to improve short circuit design of soft pack lithium battery
1198 2023-04-17
Compared with other cylindrical and square batteries, flexible packaging lithium batteries are becoming more and more popular because of their flexible size design and high energy density. Short circuit test is an effective way to evaluate flexible packaging lithium battery. By analyzing the failure model of battery short circuit test, this paper finds out the main factors that affect short circuit failure. Through the example verification under different conditions, the failure model was analyzed, and the suggestion to improve the safety of flexible packaging lithium battery was given.
The short-circuit failure of flexible packaging lithium batteries usually includes leakage, dry cracking, fire and explosion. Leakage and dry cracking generally occur in the weak area of the pole ear package. After testing, the dry cracking of the aluminum-plastic package can be clearly seen. Fire and explosion are more hazardous production accidents, and the cause is usually aluminum plastic dry crack, electrolyte reaction under certain conditions. Therefore, compared with the short-circuit test of flexible packaging lithium battery, the packaging condition of aluminum plastic material is the key factor leading to failure.
In a short-circuit test, the battery‘s open-circuit voltage drops to zero instantly, while a large current passes through the circuit and Joule heat is generated. The magnitude of joule heat depends on current, resistance and time. Although the short circuit current exists for a short time, it can still generate a large amount of heat due to the large current. This heat is released slowly after a short circuit (usually a few minutes), resulting in an increase in battery temperature. With the extension of time, joule heat is mainly lost to the environment, and the battery temperature also begins to drop. Therefore, it is speculated that the battery short-circuit failure generally occurs in the short circuit moment and a short time after.
Flexible packaging lithium batteries in short circuit testing often produce gas bulge phenomenon, this should be caused by the following reasons. The first is the instability of the electrochemical system, that is, when the high current passes through the interface between the electrode and the electrolyte, it causes the oxidation or reduction decomposition of the electrolyte, and the gas products are filled in the aluminum-plastic package. The gas production swelling caused by this reason is more obvious at high temperature, because the side reaction of electrolyte decomposition is more likely to occur at high temperature. In addition, the electrolyte may partially vaporize under the action of Joule heat even if no side reaction of decomposition occurs, especially for the electrolyte components with low steam pressure. The gas production bulge caused by this reason is relatively sensitive to temperature, that is, the bulge basically disappears when the battery temperature drops to room temperature. However, regardless of the cause of gas production, the increase in air pressure inside the battery during short circuit will aggravate the cracking of the aluminum plastic package and increase the probability of failure.
How to improve the design of soft pack lithium battery short circuit
Based on the analysis of the process and mechanism of short circuit failure, the safety of flexible packaging lithium battery can be improved from the following aspects: optimize the electrochemical system, reduce the positive and negative lug resistance, and improve the strength of aluminum-plastic packaging. The optimization of the electrochemical system can be carried out from positive and negative active materials, electrode ratio and electrolyte, so as to improve the ability of the battery to withstand instantaneous large current and short-term high heat. Reducing the resistance of the pole ear can reduce the joule heat generation and accumulation there, and greatly reduce the heat impact on the weak area of the package. Improving the strength of aluminum-plastic packaging can be achieved by optimizing the parameters in the battery manufacturing process, greatly reducing the occurrence of dry cracking, fire and explosion.
主站蜘蛛池模板: 91av在线视频免费观看 | 欧美日韩一区二区视频在线观看 | 国内成人精品视频 | 亚洲午夜精 | 欧美一区二区视频97 | 免费观看www小视频的软件 | 手机看片国产日韩 | 日韩电影中文字幕在线 | 免费在线观看av的网站 | 99热999| 中文字幕久久亚洲 | 久草视频手机在线 | 日韩在线免费视频 | www视频免费在线观看 | 91av在线免费看 | 美女视频是黄的免费观看 | 国产精品久久久久久久久久久免费 | 久久久精品影视 | 五月天综合激情 | 一区二区三区日韩视频在线观看 | 天堂网在线视频 | 一区二区久久 | 欧美日韩不卡在线观看 | 国产最顶级的黄色片在线免费观看 | 最近日本中文字幕 | 国产精品乱码久久久 | 美女视频免费一区二区 | 很黄很污的视频网站 | 欧美国产亚洲精品久久久8v | 久久久影院一区二区三区 | 成人午夜黄色 | 操操色 | 日韩中文免费视频 | 一本之道乱码区 | 91香蕉视频黄色 | 中文字幕在线观看亚洲 | 91精品办公室少妇高潮对白 | 久久久精品国产免费观看同学 | 成人免费视频观看 | 国产精品久久一区二区三区不卡 | 久久精品亚洲 | 日韩欧美视频免费在线观看 | 免费观看91视频大全 | 色成人亚洲 | 91av资源网| 在线精品一区二区 | 久草91视频 | 99久久婷婷国产精品综合 | 国产999精品久久久久久麻豆 | 精品国产亚洲一区二区麻豆 | www色,com| 日本中文字幕高清 | 超碰在线公开免费 | 日韩欧美综合视频 | 操操操日日日 | 黄色成人在线网站 | 日韩视频免费在线 | 色综合天天干 | 亚洲激精日韩激精欧美精品 | av在线播放一区二区三区 | 深爱激情婷婷网 | 在线观看中文字幕第一页 | 在线小视频国产 | av一级片网站 | 91网页版免费观看 | 日本3级在线观看 | 国产精品99久久久久久有的能看 | 成人免费观看网站 | 欧美 日韩 国产 中文字幕 | 蜜臀av.com | 久草观看视频 | 亚洲午夜久久久综合37日本 | 国产96在线观看 | av在线电影播放 | 激情视频在线高清看 | 福利视频精品 | 久久国产手机看片 | 在线播放av网址 | 亚洲午夜久久久久久久久电影网 | 精品资源在线 | 日日夜夜综合 | 天天看天天干天天操 | 97超碰人人澡 | 久久久国产网站 | 天天爽夜夜爽人人爽曰av | 久久久www成人免费毛片 | 五月天天在线 | 国产精品久久久久永久免费看 | 中文字幕免费观看视频 | 香蕉在线影院 | 黄色国产成人 | 天天爽天天爽天天爽 | 国产福利免费在线观看 | 精品一区二区在线免费观看 | 国产精品久久久久久久毛片 | 超碰九九 | 精品天堂av | 日韩欧美精品在线观看视频 | 黄色毛片在线观看 |